SUSTATEC PEEK*
Typical Properties of Stock Shapes*
| |
Property |
Units |
Test
Method |
PEEK
Unrein-
forced |
PEEK
30% Glass Reinforced |
PEEK
30% Carbon Fiber |
PEEK
Bearing Grade |
|

|
Specific
Gravity |
|
ASTM
D 792 |
1.32 |
1.51 |
1.41 |
1.44 |
| Moisture
Absorption, 24hrs |
% |
ASTM
D 570 |
0.10 |
0.10 |
0.06 |
0.05 |
| Moisture
Absorption Equilibrium |
% |
ASTM
D 570 |
0.50 |
0.50 |
0.30 |
0.30 |
| Flammability,
3.1mm sample thk |
|
UL
94 |
V-0 |
V-0 |
V-0 |
V-0 |
|

|
Tensile Strength |
psi |
ASTM D 638 |
16,000 |
15,000 |
19,000 |
15,000 |
| Tensile Elongation |
psi |
ASTM D 638 |
20 |
3 |
5 |
2 |
| Tensile Modulus |
psi |
ASTM D 638 |
500,000 |
1,000,000 |
1,250,000 |
900,000 |
| Flexural Strength |
psi |
ASTM D 638 |
25,000 |
28,000 |
26,000 |
27,000 |
| Flexural Modulus |
psi |
ASTM D 790 |
600,000 |
1,250,000 |
1,000,000 |
1,100,000 |
| Notched Izod Impact
Strength |
ft-lb/in
notch |
ASTM D 256 |
1.2 |
1.4 |
1.0 |
1.0 |
| Rockwell Hardness |
|
ASTM D 785 |
M99 |
M102 |
M102 |
— |
|

|
Heat
Deflection Temperature @ 264 psi |
°F |
ASTM
D 648 |
320 |
450 |
520 |
385 |
| Coefficient
of Linear Thermal Expansion |
in/in/°F |
ASTM
E 831 |
2.60x10-5 |
1.20x10-5 |
1.00x10-5 |
1.70x10-5 |
| Continuous
Service Temperature |
°F |
UL
746B |
464 |
464 |
464 |
464 |
|

|
Dielectric Strength |
V/mil |
ASTM D 149 |
480 |
— |
— |
— |
| Volume Resistivity |
ohm-cm |
ASTM D 257 |
1015 |
— |
104 |
— |
| Dielectric Constant @ 60 Hz |
|
ASTM D 149 |
3.3 |
— |
— |
— |
| Dissipation Factor @ 60 Hz |
|
ASTM D 792 |
0.003
|
— |
— |
— |
| Property
data is based upon testing conducted on samples fabricated from
stock shapes to better represent the characteristics of machined
parts. These values may differ from those found in resin
manufacturers’ published literature since resin property data is